X2CrNiN18-7 化學(xué)元素成分含量(%)
成分 | C | Si | Mn | P | S | Cr | Ni | N |
最小值 | - | - | - | - | - | 16.5 | 6 | 0.1 |
最DA值 | 0.03 | 1 | 2 | 0.045 | 0.015 | 18.5 | 8 | 0.2 |
X2CrNiN18-7 機(jī)械性能 | |||||
條件 | 熱處理或狀態(tài) | 抗拉強(qiáng)度 | 屈服點 | 斷后伸長率或延伸率 | 沖擊吸收能量 |
σb | σs | δ | KV2 | ||
Mpa | Mpa | % | J | ||
冷軋帶鋼:T ≤ 8mm | +AT | 650~850 | ( t ) | ( t ) | - |
Rp0.2:≥ 350①③ | T<3mm:≥35③④ | ||||
Rp1.0:≥ 380①② | T ≥ 3mm:≥40③⑤ | ||||
③ | |||||
熱軋帶鋼:T ≤ 13.5mm | +AT | 650~850 | ( t ) | ( t ) | (T>10mm) |
Rp0.2:≥ 330①③ | T<3mm:≥35③④ | I:≥ 90;t:≥60 | |||
Rp1.0:≥ 370①② | T ≥ 3mm:≥40③⑤ | ||||
③ | |||||
熱軋中厚板:T ≤ 75mm⑥ | +AT | 630~830 | ( t ) | ( t ) | (T>10mm) |
Rp0.2:≥ 330①③ | T<3mm:≥45③④ | I:≥ 90;t:≥60 | |||
Rp1.0:≥ 370①② | T ≥ 3mm:≥45③⑤ | ||||
③ | |||||
鋼材(工藝流程2H): | 冷加工+C850⑦⑧ | 850~1000 | |||
鋼材(工藝流程2H): | 冷加工+C1000⑦⑧ | 1000~1150 | |||
鋼材(工藝流程2H): | 冷加工+CP500⑦⑧ | 500~700 | |||
鋼材(工藝流程2H): | 冷加工+CP700⑦⑧ | 700~900 |